焊材:低合金钢氩弧焊条
|
ESAB 牌号
|
技术标准
|
熔敷金属力学性能
|
熔敷金属化学成分(%)
|
SFA/AWS
|
EN
|
屈服值Mpa
|
抗拉强度Mpa
|
延伸率%
|
冲击值
|
C
|
Si
|
Mn
|
Ni
|
Cr
|
Mo
|
J
|
OKTigrod 13.09
|
A5.28
|
EN 1668 W2Mo
|
424
|
560
|
31
|
+20 ℃147
|
0.1
|
0.7
|
1.1
|
-
|
-
|
0.5
|
ER80S-G
|
EN 12070 WMoSi
|
-20 ℃127
|
OKTigrod 13.12
|
A5.28 ER80S-G
|
EN12070 WCrMo1Si
|
560
|
650
|
26
|
+20 ℃180
|
0.1
|
0.7
|
1
|
-
|
1.1
|
0.5
|
OKTigrod 13.13
|
A5.28
|
EN 12534
|
570
|
710
|
24
|
0 ℃ 150
|
0.1
|
0.7
|
1.4
|
0.6
|
0.6
|
0.2
|
ER100S-G
|
WMn3Ni1CrMo
|
-40 ℃ 85
|
|
|
-60 ℃ 40
|
OKTigrod 13.22
|
A5.28 ER90S-G
|
EN12070 WCrMo1Si
|
510
|
620
|
24
|
-20 ℃200
|
0.08
|
0.6
|
1
|
-
|
2.6
|
1.1
|
OKTigrod 13.28
|
A5.28
|
EN 1668
|
540
|
630
|
30
|
-20 ℃200
|
0.1
|
0.6
|
1.1
|
2.4
|
-
|
-
|
ER80S-Ni2
|
W2Ni2
|
-40 ℃180
|
|
|
-60 ℃150
|
OKTigrod 13.32
|
A5.28 ER80S-6B
|
EN 12070 WCrMo5
|
580
|
680
|
22
|
+20 ℃200
|
0.07
|
0.4
|
0.5
|
0.2
|
5.7
|
0.6
|
|